PolyBeskar 730®

Explaining PolyBeskar 730®

Let’s use a visual aid to explain

Many of us have heard or seen a presentation about the professor who fills a mayonnaise jar with large rocks and asks if it’s full, then slowly adds smaller and smaller material until finally filling the remaining space with liquid.

PolyBeskar 730® works in a similar fashion.

The material starts with a low atomic density, ultralight material, then fills in the gaps between the atoms with other ultralight materials- slowly adding more structure and creating a network of intermixed atoms that recombine into a new form that is bonded as a final unit in a binary liquid resin.

Just like concrete, once PolyBeskar 730® is mixed and cured it goes from a liquid state to a solid and doesn’t go back.

In its finished form, PolyBeskar 730® is incredibly light in weight, yet remarkably high density.

While in its resin state, various materials can be added in order to achieve varying desired properties such as carbon, ceramic and other nano-fibers.

The possibilities for use are nearly endless.

Polybeskar is a standalone material that can be used alone or in conjunction with various additives and fiber materials for increased, enhanced, or alternative properties.

Properties may be tailored through formulation, reinforcement, and additive selection.

This material can easily be used in most instances as an alternative to aluminum at approximately 60% less weight. It can be cast, molded, extruded, pultruded, blow formed, machined, and more…

General Specs & Cure details:

Specific gravity: ≈1.12 g/cm³ density

• Viscosity;

A. 1500-2000 cps

B. 350-450 cps

C. 780 combined @ 77oF

• Epoxy Equivalent Weight; B. 131– 143

• Anhydride Molecular Weight; A. 235-245

• Mixed Volume/Weight A. 9.38lbs/gallon

• Gel Time;

@ 212°F / 23 minutes

@ 320°F / 90 seconds

• Full Cure; 60 minutes @ 350°F*

• TGbyDMA; 245°C

• Heat Distortion: 210°C

• Tensile Strength: Neat Resin ≥30,000 psi

• Tensile Elongation: 2.7%

• Tensile Modulus: 215,000 psi

• Fracture Toughness: 730psi/in1/2

Mix ratio:

Part A – 100 parts by weight (Clear liquid resin)

Part B – 160 parts by weight (Amber color liquid) This mix ratio is critical to maintain the physical properties of the resin system.

Stir/mix parts A & B together to blend the components. Use low to medium RPM, low shear, mixing equipment, when blending the resin system. A High Speed or Shear mixer may generate exothermic heat build- up and shorten pot life, especially in larger mix batches.

Resin bath should be kept at 75°F to 85°F.

Mixed Pot Life:

8-hrs at 77°F (25°C) =1,560 cps 24-hrs at 77°F (25°C) = 5,000 cps Higher temperatures will shorten the pot life.

If the pot life needs to be extended; The mixed resin can be stored under refrigeration in a sealed container.

Allow the resin to return to room temperature before use, especially after being refrigerated, to help prevent any condensation build up, (dependent on relative humidity).

Cleanup of tools or other surfaces can be accomplished with MEK or other similar solvents. PolyBeskar 730® resin system cont’d;

Curing options:

The PolyBeskar 730® resin system can be processed in standard mold operations utilizing nanoparticle fillers such as; silica fused whiskers, graphene, boron nitride, among others, allowing for custom properties to be built into the resin system, including custom doping of other various materials.

— or

The PolyBeskar 730® resin system can be extruded, pultruded or blow formed, in combination with Carbon Fiber strands, Basalt Fiber strands or other hardened core materials. Other additive materials can be included to provide additional material properties as needed. Then these cured resin rods of various diameters can be CNC machined to specific lengths and tip shapes to best fit the intended use.

*Other options to consider; for faster cure times addition of accelerator chemistry can be added, though testing for the final ratio blend must be done to determine the required finished product properties for its intended use.

Required Mold release: It is strongly suggested to use the JTI-2640 nano-ceramic release coating when curing this resin system in mold cavities to ease removal and better surface properties. 

General Specs & Cure details:

1. Resin Classification & Chemistry

Base Chemistry:

• High-grade aerospace polyimide thermoset

• Modified for increased molecular density and above-average processing ease.

Molecular Architecture:

• Ultra-high molecular density polyimide backbone with various copolymers in an ultra

dense matrix.

• Designed for low cure strain and low thermal strain

• Supports staged conversion (B-stage) and multi-route manufacturing.

2. Rheology & Viscosity (77°F / 25°C)

Viscosity (formulation-dependent):

• Low-flow formulation: 350–450 cP

• High-build formulation: 1,500–2,000 cP

• Blended nominal viscosity: ~780 cP @ 77°F

This tunable viscosity range supports casting, injection molding, compression molding, fiber

impregnation, extrusion, and pultrusion processes.

3. Density & Mass Properties

Mixed/Cured Density:

• ~9.38 lb/gal (≈1.12 g/cmÑ, ≈18.4g/inÑ)

This density enables lightweight structural composites and supports near-zero dimensional

change across cure and thermal cycling.

4. Cure Kinetics & Processing Window

Gel Time (per 0.5 inch sec=on thickness):

• 212°F (100°C): ~23 minutes

• 320°F (160°C): ~90 seconds

Typical Full Cure:

• 60 minutes @ 350°F (177°C)

• Optional post-cure cycles may be used to further increase Tg and thermal

stability

B-Staging:

• Resin supports partial cure into pellets, billets, preforms, filament, tape, and pultruded

intermediates.

5. Thermal Properties (Neat Resin)

Glass Transition Temperature (DMA, neat resin):

• ≥245°C (baseline)

• Higher Tg achievable with extended or elevated post-cure

Thermal / Dimensional Stability:

• <0.001% strain @ ≥210°C

• Near-zero cure shrinkage and thermal expansion when properly processed

6. Mechanical Properties

Tensile Strength (Representative):

Neat Resin:

• ≥30,000 psi

Carbon Fiber Reinforced (PolyBeskar Resin System):

• Near-isotropic CF composite: ≥48,000 psi

• Unidirectional / isolinear CF: ≥105,000 psi

Basalt Fiber Reinforced:

• Near-isotropic basalt composite: ≥125,000 psi

• Unidirectional / isolinear basalt: ≥263,000 psi

Note: Composite values depend on fiber type, volume fraction, architecture, void content,

and processing method.

Tensile Elongation (Neat Resin):

• ~2.7%

Tensile Modulus (Neat Resin):• ~215,000 psi

Composite modulus is fiber-dominated and architecture-dependent.

7. Fracture & Damage Tolerance

Fracture Toughness (Mode I, representative):

• ~730 psi·inÅᐟÇ

This toughness level supports reduced microcracking, improved fatigue resistance, and

enhanced thermal-cycling durability.

8. Exotherm Characteristics

Lower-Temperature Cure Profile:

• Peak exotherm =me: ~38 minutes @ 194°F

• Peak exotherm temperature: ~199°F

Accelerated Cure Profile:

• Peak exotherm =me: ~2.82 minutes @ 338°F

• Peak exotherm temperature: ~453°F

Dual exotherm regimes allow controlled thick-sec=on curing or rapid thin-section

processing.

9. Reinforcement & Additive Compatibility

PolyBeskar is compatible with carbon, basalt, glass, aramid, and specialty fibers, as well as

functional nano-materials and fillers. These additives may be used to tailor strength,

stiffness, thermal behavior, fire response, electrical properties, impact resistance, and

fatigue life.

10. Fire & Thermal Response

Under intense localized heat or flame exposure, PolyBeskar forms a carbonaceous foamed

char layer that acts as a thermal barrier, slowing heat transfer and protecting underlying

structures. This response is localized and preserves surrounding material integrity.

Mix ratio:

Part A – 100 parts by weight (Clear liquid resin)

Part B – 160 parts by weight (Amber color liquid) This mix ratio is critical to maintain the

physical properties of the resin system.

Stir/mix parts A & B together to blend the components. Use low to medium RPM, low shear,

mixing equipment, when blending the resin system. A High Speed or Shear mixer may

generate exothermic heat build- up and shorten pot life, especially in larger mix batches.

Resin bath should be kept at 75°F to 85°F.

Mixed Pot Life:

8-hrs at 77°F (25°C) =1,560 cps

24-hrs at 77°F (25°C) = 5,000 cps Higher temperatures will shorten the pot life.

If the pot life needs to be extended; The mixed resin can be stored under refrigeration in

a sealed container. Allow the resin to warm up to before using, aver being refrigerated, to

help prevent any condensation build up, (dependent of Relative Humidity).

Cleanup of tools or other surfaces can be accomplished with MEK or other similar solvents.

Notes on Curing and Handling Options:

The Polybeskar® Resin system can be processed in standard mold operations utilizing

nanoparticle fillers such as; silica fused whiskers, graphene, boron nitride, among others,

allowing for custom properties to be built into the resin system, including custom doping of

other various materials.

— or

The PolyBeskar® resin system can be extruded, pultruded or blowformed, in combination

with Carbon Fiber strands, Basalt Fiber strands or other hardened core materials. Other

additive materials can be included to provide additional material properties as needed.

Then these cured resin rods of various diameters can be CNC machined to specific lengths

and tip shapes to best fit the intended use.

*Other options to consider; for faster cure times addition of accelerator chemistry can be

added, though testing for the final ratio blend must be done to determine the required

finished product properties for its intended use.

Required Mold release: It is strongly suggested to use the 2640 nano-ceramic release

coating when curing this resin system in mold cavities to ease removal and better surface

properties.

Manufacturer is not responsible for the use and application of this material. It is up to

the end user to determine the suitability of this product for their own application. It is the

belief that the contents of this document were accurate at the time of printing. No

warranty is written or implied regarding application and use of this product.

PolyBeskar 730® Applications

Images and products displayed on this site may not contain proprietary material developed by PolyForge Industries, LLC. and are displayed for demonstration purposes only.